How Should the Thermal Resistance of Tungsten-Copper Heat Sinks in Power Modules Be Evaluated Under High-Current Conditions?

tungsten copper heat sink thermal resistance
power module junction-to-case thermal resistance testing
JESD51-14 transient thermal impedance measurement
high-current IGBT MOSFET heat sink evaluation
MIM tungsten copper heat spreader for power modules
applications

Published:

How Should the Thermal Resistance of Tungsten-Copper Heat Sinks in Power Modules Be Evaluated Under High-Current Conditions? / 功率模块钨铜热沉在大电流工况下的热阻表现如何评估?

How Should the Thermal Resistance of Tungsten-Copper Heat Sinks in Power Modules Be Evaluated Under High-Current Conditions?

Evaluate a tungsten-copper (W-Cu) heat sink as one layer in a standardized thermal stack. Your test plan should produce four types of evidence:

1. Junction-to-case thermal resistance. Measure Rth(j-c) with the transient dual interface method in JEDEC JESD51-14. 2. Transient thermal impedance. Record the full Zth(t) curve, because high-current pulses are limited by transient behavior as well as by steady-state resistance. 3. Material and interface data. Confirm thermal diffusivity of the W-Cu by laser flash (ASTM E1461) and characterize interfaces separately (ASTM D5470). 4. Stability under cycling. Repeat the Rth measurement before and after power cycling (IEC 60749-34, or ECPE AQG 324 for automotive modules).

A catalogue conductivity value does not describe heat-sink behavior under high current. A traceable measurement chain built on recognized standards can.

Where the Heat Sink Sits in the Thermal Path

Under high current, heat is generated in the die. For a MOSFET, conduction loss is roughly I²·R_DS(on). For an IGBT, it is roughly V_CE(sat)·I. Switching losses add to both. R_th,j-c sums the layers from the junction to the case surface, including a W-Cu baseplate or internal spreader on that path. A sink mounted after the case, plus the TIM and cold plate, sits in the system resistance.

A first-order one-dimensional model is:

R_th,j-c ≈ Σ tᵢ / (kᵢ · A_eff,i), and ΔT_j(t) = P_loss · Z_th(t)

In this model, t is layer thickness, k is thermal conductivity, and A_eff is the effective heat-spreading area at that layer.

Design and purchasing implications:

- Find the dominant term first. The baseplate is one term in R_th,j-c. When solder or the external TIM dominates, a higher-conductivity grade adds cost and little temperature reduction. - Spreading area matters. A_eff grows as heat spreads laterally. A heat sink thick enough to spread the heat can lower total Rth even when its own conduction term increases. - Use the right metric for pulses. Short high-current events are governed by Z_th(t). Thermal mass of the W-Cu layer affects the curve after the die and die attach have responded. Specify Rth and Zth at the pulse widths the inverter or driver actually uses. - Treat the model as a sizing tool. Use it to set targets and choose thickness. Use measured values to accept parts.

Standards That Make a Thermal Resistance Number Defensible

The table below matches each evaluation question to a recognized method. Numbers from module makers and heat sink suppliers are comparable only when both sides measured the same boundary.

Evaluation question Reference standard What it measures Role for a W-Cu heat sink Limitation
Junction temperature sensing JEDEC JESD51-1 Electrical test method; K-factor calibration of a temperature-sensitive parameter Gives a traceable Tj under heating current Calibration drifts if sense current or fixture changes
Junction-to-case resistance JEDEC JESD51-14 (transient dual interface) Rth(j-c) from two Zth curves taken with different case interfaces Separates the path to the case; includes W-Cu when that part lies on the path Single heat-flow path; the two interfaces must differ only at the case
Bulk material property ASTM E1461 (laser flash) Thermal diffusivity; conductivity follows with density and specific heat Lot-level check of diffusivity for the W-Cu grade Coupon geometry, not the finished part
Interface resistance ASTM D5470 Steady-state resistance of TIMs and interfaces Separates mounting losses from heat sink performance Results depend on pressure and flatness
Power device ratings IEC 60747-9 / IEC 60747-15 Definitions and test conditions for IGBTs and isolated modules Fixes how Rth is reported on the datasheet Device-level scope
Degradation under load IEC 60749-34; ECPE AQG 324 Power cycling, with Rth or V_CE drift as a failure criterion Shows whether the stack stays stable Long test duration
Hermetic and military packages MIL-STD-883, Method 1012 Thermal characteristics of microcircuits Relevant for hermetic W-Cu packages Narrower scope than commercial power modules

JESD51-12 sets out how to report thermal data. Ask suppliers to follow it so their numbers state the boundary conditions behind them.

Test Conditions That Change the Result at High Current

The same heat sink can give different Rth values when conditions shift. Record each of the following in the test report:

- Heating power and duration. Hold heating long enough to reach steady state for Rth. For Zth, sweep pulse widths from microseconds to seconds. - Temperature sensing. Keep the sense current low and constant, and recalibrate the K-factor whenever the device or fixture changes. - Cooling boundary. Record coolant temperature, flow rate and cold-plate flatness. In JESD51-14, the two case interfaces must differ only at the case surface. - Mounting. Record clamping force or screw torque. Mounting pressure changes the TIM contribution to system temperature rise, so record it with the interface conditions. - Attach quality. Inspect solder or sintered joints by X-ray before thermal testing. Voids directly under the die raise local Rth, and that increase can be wrongly blamed on the heat sink.

Material and Manufacturing Variables to Audit

Grade selection balances conductivity against thermal expansion (CTE). W70Cu30 and W80Cu20 are the usual choices for heat spreaders that must match the CTE of semiconductor dies. The grade range covers W70Cu30 to W90Cu10, and copper content can be customized from 6–90 wt%.

Three manufacturing outcomes have a direct effect on the measured Rth:

- Densification. Residual porosity lowers effective conductivity and reduces lot-to-lot repeatability. - Flatness. Flatness after sintering and plating sets the bond-line thickness of the solder or TIM against the part. - Surface finish. Au/Ni plating should remain compatible with soldering or bonding.

A practical acceptance package therefore combines three items: laser-flash coupons from the same powder and sintering lot, flatness maps of the finished parts, and JESD51-14 results on a reference module.

Production route also matters. MIM forms small heat sinks with micro-channels, cavities or thin walls. Pressing and copper infiltration are also used for W-Cu plates.

Applicability Limits of the W-Cu Term

- The heat sink term is small. If Rth is dominated by the substrate or TIM, adjust those layers first. - The pulses are very short. At pulse widths set by the die and the die attach, Z_th is insensitive to the W-Cu layer. - Rth drifts after power cycling. This points to the attach layer or a CTE mismatch, and both need correction at the stack level.

Supplier Evidence That Supports the Measurement Chain

Newlife - MIM produces W-Cu heat sinks, heat spreaders and substrates for power electronics. The following capabilities can be traced through documentation:

- Process control. Parts are formed by MIM/PM near-net-shape processing and sintered to ≥98% relative density, which keeps mechanical properties close to wrought material. - Raw material traceability. Tungsten powder is developed in-house. - Geometry. Micro-channels and thin walls can be formed near-net; mounting pads are machinable, with Au/Ni plating and soldering compatibility. - Quality system. Production runs under IATF 16949, ISO 9001 and ISO 14001. Lot traceability under these systems supports automotive PPAP submissions. - Development support. For new module designs, joint OEM/ODM development and rapid prototyping allow JESD51-14 testing on representative parts before tooling is frozen.

Next Steps

1. Build the junction-to-case stack model and identify which layer dominates Rth(j-c). 2. Define Zth pulse widths from the real mission profile of your inverter or driver. 3. Specify JESD51-14 testing with documented boundary conditions, reported according to JESD51-12. 4. Request ASTM E1461 coupons, flatness data and plating specifications for each lot. 5. Repeat Rth measurements after IEC 60749-34 or AQG 324 power cycling. 6. Contact Newlife - MIM for application-specific engineering support. Visit http://www.newlife.cn/ to request a free consultation, share your module stack and current profile, and get prototype W-Cu heat sinks for your thermal resistance validation program.

References

1. JEDEC JESD51-1, Integrated Circuits Thermal Measurement Method – Electrical Test Method (Single Semiconductor Device). 2. JEDEC JESD51-12, Guidelines for Reporting and Using Electronic Package Thermal Information. 3. JEDEC JESD51-14, Transient Dual Interface Test Method for the Measurement of the Thermal Resistance Junction-to-Case of Semiconductor Devices with Heat Flow Through a Single Path. 4. IEC 60747-9, Semiconductor devices – Discrete devices – Part 9: Insulated-gate bipolar transistors (IGBTs). 5. IEC 60747-15, Semiconductor devices – Discrete devices – Part 15: Isolated power semiconductor devices. 6. IEC 60749-34, Semiconductor devices – Mechanical and climatic test methods – Part 34: Power cycling. 7. ECPE Guideline AQG 324, Qualification of Power Modules for Use in Power Electronics Converter Units in Motor Vehicles. 8. ASTM E1461, Standard Test Method for Thermal Diffusivity by the Flash Method. 9. ASTM D5470, Standard Test Method for Thermal Transmission Properties of Thermally Conductive Electrical Insulation Materials. 10. MIL-STD-883, Method 1012, Thermal Characteristics. 11. Lutz, J., Schlangenotto, H., Scheuermann, U., De Doncker, R., Semiconductor Power Devices: Physics, Characteristics, Reliability, Springer. 12. Newlife - MIM, Tungsten Copper Heat Sink product page, http://www.newlife.cn/zh/products/tungsten-copper-heat-sink

Back to Blog

Have a Part Design? Let's Evaluate It for MIM.

Send us your 2D/3D drawings — our engineers will respond with a feasibility assessment and quotation.