How Can Warpage of Small IGBT Module Heat-Sink Bases Be Controlled? Copper and Tungsten-Copper Sintering and Flattening Processes
Published:

How Can Warpage of Small IGBT Module Heat-Sink Bases Be Controlled? Copper and Tungsten-Copper Sintering and Flattening Processes
Warpage in a small IGBT heat-sink base is controlled at three points. First, keep the shrinkage strain uniform through the thickness during sintering, using balanced geometry, uniform green density, and proper support. Second, pick the material route by how well it holds shape at temperature. Tungsten-copper keeps a rigid tungsten network, while pure copper softens and sags. Third, correct any remaining bow with a flattening step that actually goes beyond the material's elastic limit. A simple bending model shows why room-temperature pressing often fails on thin copper bases, and when hot flattening or lapping is the better correction.
Where Warpage in Sintered Heat-Sink Bases Comes From
A sintered base bows when one face shrinks more than the other. In MIM, linear shrinkage from the moulded state is large, so small gradients in green density, binder content, temperature, or friction against the setter become measurable curvature. In an IGBT module, the solder or sinter layer to the DBC substrate amplifies the problem. The base must be flat, or have a controlled bow, to keep bond-line and thermal-interface thickness uniform.
Two effects add to sintering distortion:
- Gravity sag. It is severe for pure copper sintered close to its melting point, and it grows with unsupported span. - Thermal-expansion mismatch with the substrate after assembly. W–Cu helps here because its coefficient of thermal expansion can be tailored toward semiconductor and ceramic materials.
Curvature From a Through-Thickness Shrinkage Gradient
Treat the base as a plate of thickness t whose shrinkage strain varies linearly from one face to the other by Δε. For free cylindrical bow, at small deflection relative to span L, the curvature and centre deflection are as follows. Δε is entered as a fraction, and t and L use the same length unit.
κ = Δε / t
δ = κ·L² / 8 = Δε·L² / (8t)
The model gives three practical levers:
- Span dominates. Deflection scales with L², so doubling the base length quadruples the bow for the same process gradient. Long bases need tighter density control or a planned flattening allowance. - Thickness helps linearly. Thinning a base to cut thermal resistance raises warpage risk proportionally. Thin designs should be paired with a material that resists creep at sintering temperature. - Δε is the process variable. Uniform powder size distribution, homogeneous feedstock, symmetric gating, and flat ceramic setters all act on Δε directly. This is where powder and compounding control pay off.
Why Room-Temperature Sizing Often Springs Back
Pressing a bowed base flat imposes a surface bending strain of κ₀·t/2. The press is fully elastic, and the bow returns on unloading, when that strain stays below the yield strain. Surface yield starts when:
κ₀·t/2 > σᵧ / E
Sintered copper is soft, but on a thin base the bending strain is small, so a flat press often leaves the bow in place after unloading. Practical consequences:
- Copper bases need reverse over-bending in a sizing die with slight counter-camber, or a flattening anneal under load, with the parts held between flat plates at elevated temperature in a protective atmosphere so that creep relaxes the curvature. - Small residual bows on thin parts are removed by lapping or grinding of the mounting face, provided machining stock was planned into the near-net design. - For W–Cu, the usual corrections are hot flattening, controlled-atmosphere annealing under weight, precision lapping, or mirror grinding of the interface face.
Copper vs Tungsten-Copper Routes for Flatness
| Route | Shape-holding during sintering | Main warpage driver | Effective flattening options | Best fit |
|---|---|---|---|---|
| Pure copper MIM | Low; copper softens near its melting point and sags under its own weight | Gravity sag, density gradients, setter friction | Over-bend sizing, flattening anneal under load, lapping | Highest thermal conductivity; small spans, thicker sections, complex fins or channels |
| W–Cu MIM (liquid-phase sintering) | High; the tungsten network carries load while copper is liquid | Tungsten distribution and uneven shrinkage | Hot flattening, lapping or grinding | Thin bases needing CTE matching and near-net micro-channels or steps |
| W–Cu pressing / isostatic pressing + sintered W skeleton + Cu infiltration | Very high; the pre-sintered skeleton fixes geometry before infiltration | Skeleton density uniformity, infiltration completeness | Grinding or lapping of mounting faces | Simpler, flatter plates where geometric complexity is low |
Common grades for these heat spreaders and heat sinks are W70Cu30 and W80Cu20. Copper fraction and tungsten fraction are chosen so expansion can be matched to the semiconductor or ceramic while conductivity stays high.
Design Window for Low-Warpage Bases
- Balance the cross-section. Put fins, pins, or cavities symmetrically about the mid-plane, or add balancing ribs on the opposite face. An asymmetric section creates its own Δε. - Set nominal thickness by span. The δ ∝ L²/t relation shows how span and thickness trade off against a flatness budget. Confirm the thickness in trial sintering before freezing the design. - Specify flatness and bow direction together. Many IGBT assemblies prefer a slight convex bow toward the cooler so that clamping closes the interface. Defining the sign of the bow lets the flattening step target it. - Reserve stock only where needed. If the mounting face will be lapped, add stock there and keep all other features net-shape. - Plan plating early. Ni/Au and Ni/Ag finishes, and later brazing or soldering, add thermal cycles. Flatness should be verified after the final heat-related step.
When MIM Is a Poor Fit
MIM is a poor fit for very large, flat, featureless plates, because deflection grows with L² and warpage control dominates the process. Abrupt wall-thickness steps can cause debinding cracks and density gradients. In pure copper, oxygen pickup and incomplete densification reduce conductivity, so atmosphere and residual carbon and oxygen have to be controlled. If the shrinkage spread cannot be held inside the dimensional tolerance band, a machined or hybrid route is the practical choice.
How Newlife - MIM Addresses Each Lever
Newlife - MIM produces chip heat-sink bases in pure copper and W–Cu by MIM/PM near-net shaping, with sintered relative density ≥ 98 % and mechanical properties close to wrought material. The bases are made for low warpage and stable flatness, matched thermal expansion, and plating, soldering and bonding. W–Cu baseplates hold flatness in thin sections and can carry multi-level, groove and step features.
Each warpage lever maps to a process control:
- Δε starts with powder. The company develops and produces its own ultrafine copper, iron and nickel powders (D50≤3μm), and its own tungsten powder for W–Cu heat spreaders. Particle size distribution, morphology and purity are controlled for consistent sintering behaviour. - One process chain. Feedstock compounding, granulation, moulding, debinding, sintering and post-processing run in-house, so a flatness deviation can be traced to the specific lot and step. - Several W–Cu routes. Both MIM and isostatic pressing with a sintered tungsten skeleton and copper infiltration are available, so geometry can drive the route choice. - Dimensional control. Near-net-shape tolerance is ±0.3 %–0.5 %.
Next Steps
1. Use δ = Δε·L²/(8t) with Δε from trial shrinkage, together with span and thickness, to rank flatness risk before freezing the section. 2. Decide between copper, W70Cu30 and W80Cu20 from the substrate CTE and the thermal budget. 3. Define the flatness value, bow direction and the post-plating measurement point on the drawing. 4. Request trial sintering with flatness data before and after sizing or lapping, plus density and conductivity checks. 5. Contact the Newlife - MIM application engineering team for OEM/ODM development and rapid prototyping of the IGBT heat-sink base. Visit http://www.newlife.cn to send drawings.
References
1. German, R. M., & Bose, A. Injection Molding of Metals and Ceramics. Metal Powder Industries Federation, 1997. 2. German, R. M. Sintering Theory and Practice. Wiley, 1996. 3. ASM International. ASM Handbook, Volume 7: Powder Metallurgy. 4. MPIF Standard 35. Materials Standards for Metal Injection Molded Parts. Metal Powder Industries Federation. 5. Newlife - MIM. Power electronics and chip heat-sink base product pages. http://www.newlife.cn